Home›Problems and fixes›Cracks
Wall cracks · read before you fill

Is this crack in the plaster or in the structure? Read its place, shape and width

The short answer
  1. Where is it?A net of fine lines in the plaster, or a straight line along a joint (wall to column, wall to beam or slab), is usually the plaster or normal movement. A crack in a beam, column or slab, or one running across the brickwork from a corner, is the structure.
  2. What shape?Map-like: the plaster shrank. Straight and even: two materials moved apart. Diagonal, stepped like a staircase, or wider at one end: part of the house has settled.
  3. How wide?Under 1 mm is a hairline. Over 3 mm, an engineer sees it before anyone fills it.

One rule sits over all three: a crack that comes back after filling is still moving. Stop filling it.

< 1 mm
HairlineUltraTech calls these usually cosmetic, common in new plaster.
3 mm
Engineer firstThe line UltraTech and Dr. Fixit both give.
4 cards
Quick checkFour ATM cards held together are about 3 mm thick.
Where the crack sits tells you what moved
One wall of a framed house with six kinds of crack marked A: a net of fine lines in the plaster (fill it). B: a straight vertical line where the wall meets the column (fill with mesh). C: a straight horizontal line under the roof slab and beam (watch, then fill). D: a short thin diagonal from the corner of the window lintel (watch, then fill). E: a long stepped diagonal from the window corner down towards the floor, wider at the top (engineer first). G: fine cracks in the underside of the beam (engineer first). ROOF SLAB AND BEAM FLOOR COLUMN COLUMN A B C D E G Fill it Watch, then fill Engineer first F and H are on the cards below: they need a whole wall or time to show.
Causes from BIS SP 25, Handbook on causes and prevention of cracks in buildings. Widths drawn larger than life.
Find your crack

Eight cracks, and what each one is telling you

Match yours to a card. The colour says whether you can fill it. If it fits two cards, go by the redder one.

A

A net of fine lines in the plaster

Plaster only · fill it

The plaster dried too fast, the mix was too rich in cement, or it was not kept wet long enough. SP 25 puts this under shrinkage. It does not travel into the brick.

Do: open the lines lightly, fill with putty, then paint. See cracks in plaster and cracks before painting.

COLUMN brick and concrete move differently
B

A straight line where the wall meets a column

Joint movement · fill with mesh

Concrete and brick shrink and swell by different amounts, so the joint between them opens. In framed houses this is the commonest crack of all.

Do: open it into a V, SBR-cement mortar, a strip of fibre mesh across the joint, then putty. Putty alone will crack again on the same line. Over 3 mm, or the column itself cracked: engineer.

top floor, under the roof
C

A straight line just under the roof slab or beam

Slab movement · watch, then fill

The roof slab heats in the sun and grows more than the wall below it. SP 25 describes this crack in top-floor rooms. It opens and closes with the seasons.

Do: fill with something that can move (SBR mortar and mesh), and keep the roof dry and cooler from above: terrace waterproofing. Wall pushed out, or wider than 3 mm: engineer.

D

A short, thin diagonal from a window or door corner

Corner stress · watch, then fill

The corners of an opening gather stress, and the plaster meets the lintel and frame there. A short, thin crack that stops after a hand's length is usually this.

Do: watch it for a month; if it stays the same, fill with a crack filler or SBR mortar and mesh. More on cracks at window and door corners.

wide
E

A long diagonal or stepped crack, wider at one end

Settlement · engineer first

One part of the foundation has gone down more than the rest. It often runs from an opening towards a corner of the house, and doors or windows near it start to stick. In north Bihar, soil that floods and dries again is a common cause.

Do: don't fill it. See house settling on one side.

bulge
F

A horizontal crack along a load-bearing brick wall

Wall under load · engineer first

In an older house with no columns, the brick walls carry the roof. A crack running along the middle of such a wall, or a wall that looks pushed out when you sight along it, means it is carrying more than it can.

Do: keep weight off that floor and call an engineer.

BEAM
G

A crack in a beam, column or slab itself

Frame · engineer first

These carry the house. Cracks across the underside of a beam, a slanting crack near its ends, or any crack with brown rust marks along it, are not plaster problems.

Do: engineer first. Rust and falling concrete: steel showing through the slab.

filled in March back by August
H

A crack that comes back after filling

Still moving · stop filling

The filler was fine. Whatever opened the crack is still at work, and every filling hides the evidence an engineer needs.

Do: stop filling, mark its ends with a date and watch it: is the crack still moving?

The test that settles it

Plaster only, or the wall behind it?

Plaster is a skin about 12 to 20 mm thick. These four checks tell you whether the crack stops in the skin or goes on into the brick and concrete.

1Scrape a little

Chip the plaster off for a hand's length along the crack with a chisel. Bricks and joints whole behind it: plaster crack. Crack carries on through the joints or bricks: it is in the wall. Patch the plaster afterwards.

2Look at the other face

Find the same spot on the other side of the wall, in the next room or outside. A crack that shows on both faces goes right through the wall. Light or air through it: call an engineer today.

3Tap around it

Tap the plaster with a coin or a screwdriver handle. A hollow sound means the plaster has come away from the wall. That patch needs re-plastering, not filling: cracks in plaster.

4Check it is flat

Lay a ruler or a straight stick across the crack. If one side stands out further than the other, the wall has moved sideways. That is never shrinkage: engineer first.

The scrape test
Two walls with a patch of plaster chipped off along the crack Left: behind the chipped plaster the bricks and joints are whole, so the crack was only in the plaster. Right: the crack carries on through the brick joints, so it is in the wall. Bricks whole: plaster crack Goes into brick: wall crack
Chip only a hand's length. On a beam or column, don't chip: show it to an engineer as it is.
Measure the width

How wide is it? Use an ATM card, or print our card

Width alone doesn't decide (Asian Paints says the same: a thin crack can be structural). But it tells you how soon to act. An ATM card is 0.76 mm thick, the same size everywhere.

What goes into the crackWidthReading
Nothing; it looks like a drawn hairNot even one card's edge< 1 mmHairline. Usually the plaster. Fill it, if the place card agrees.
One or two ATM cardsSlide the edge in gently1–2 mmGo by the place card. Crack filler or SBR mortar if it is green or yellow.
Three cards togetherA little over 2 mm2–3 mmWatch it for a month before filling. Measure in the same spot.
Four cards togetherAbout 3 mm> 3 mmEngineer before filling. UltraTech and Dr. Fixit both draw the line here.
A fingertip, or light shows throughmuch moreCall today. Keep people away from that wall.
The makers don't all say the same. UltraTech's tip and FAQ say a crack over 3 mm needs a professional, but its repair steps only send you for help above 1 cm. Dr. Fixit says 3 mm. Birla White sells Crack End for non-structural cracks up to 5 mm. We use the safest of these: over 3 mm, an engineer sees it first, even if Crack End is what goes in afterwards.
Crack-width card, to print
Printable crack-width card Black bars 0.3, 1, 2, 3 and 5 mm wide. Up to 1 mm: plaster, fill. 1 to 3 mm: check the place. 3 mm and more: engineer first. A 50 mm line checks the print size. Lines to write the date, place and width. CRACK WIDTH CARD tashyaventures.com · 90310 74624 0.31235 mm PLASTER · FILL CHECK PLACE ENGINEER FIRST This line must be 50 mm.If not, print again at 100%. Date ______ Place on wall ______________ Width ____ mm Date ______ Place on wall ______________ Width ____ mm Date ______ Place on wall ______________ Width ____ mm
Print at 100%, cut it out, and hold the bars against the crack. Photograph the card beside the crack each time and keep the photos with their dates.
For the green and yellow cracks

What fills which crack, and how

Only once the crack has passed the place card, the scrape test and the width check. Full method: sealing cracks and joints.

CrackFill with
Hairline net in the plaster (A)under 1 mm, insideBirla White WallCare putty, after opening the lines lightly. Birla White says putty fills minor cracks.
Hairline on an outside or damp wallunder 1 mmBirla White Waterproof putty, once the wall is dry.
Plaster crack 1–3 mm, not at a jointA or D, steadyBirla White Seep Guard Crack End: a white-cement crack filler for non-structural cracks, rated to 5 mm. We can order it for you.
Joint cracks: column, beam, slab (B, C)and steady cracks deeper than the plasterSBR-cement mortar with UltraTech Seal & Dry SBR, and a fibre mesh strip across the joint.
Outside wall where rain gets inany of the above, outsideRepair mortar with WP+200 in it, then exterior primer and paint.
Things we see go wrongCement slurry smeared over the top: it sits on the surface and cracks again within weeks. Putty pushed into a wide crack: putty is a skin, not a filler. A joint crack filled without mesh: back on the same line next summer. And the worst one: a red-card crack filled and painted the week before a wedding, so nobody can read it later.
  1. Photograph and date itWith the width card beside it. If it comes back, these photos are what the engineer will ask for.
  2. Open it into a VWith a chisel or a cutter along the crack, so the filler has sides to grip. Knock off any loose or hollow plaster around it.
  3. Clean and wet itBrush out all dust. Dampen the groove, with no water standing in it.
  4. FillPutty or Crack End for plaster cracks. For joints: a slurry coat of SBR and cement first, then SBR-cement mortar pressed in hard. Mix as the pack says.
  5. Mesh across jointsPress a strip of fibre mesh into the fresh coat across any wall-to-column or wall-to-slab crack, a few fingers wide on each side.
  6. Cure, then finishKeep mortar repairs damp for a few days (UltraTech says 3 for concrete repairs). Then putty, primer and paint in the right order: putty, primer, paint.
Red cards

When an engineer sees it before anyone fills it

  • Wider than 3 mm (four ATM cards go in)
  • Diagonal or stepped across the brickwork, or wider at one end
  • In a beam, column or slab, or with rust marks along it
  • One side of the crack stands out from the other
  • It shows on both faces of the wall, or you see light through it
  • Doors or windows near it have started to stick
  • New cracks in several rooms at once, or after a floor was added on top
  • It came back after it was filled

Until the engineer comes, don't fill or paint over it. The engineer reads the crack: its line, its width, which way it is wider. A fresh coat of putty wipes all of that off.

Engineers and architects we can point you to are on our engineers page. To tell whether it is still moving, use the pencil-mark and paper-strip test on is the crack dangerous?

Not sure which card it is? Send us photos on WhatsApp, with the width card or an ATM card beside the crack and one photo of the whole wall, and we will look at them with you.

Questions people ask us

Short answers

How do I tell if a wall crack is in the plaster or the structure? (darar plaster ki hai ya dhanche ki)

Scrape the plaster off for a hand's length along the crack. If the bricks and mortar joints behind are whole, the crack was in the plaster only. If it carries on through the bricks or joints, or shows on the other face of the wall, it is in the wall itself.

How wide a crack needs an engineer?

Wider than 3 mm, which is about four ATM cards held together. UltraTech and Dr. Fixit both put the line at 3 mm. Also call for any crack that grows, comes back after filling, or sits in a beam, column or slab, whatever its width.

Why is there a straight crack where the wall meets the column?

Concrete and brick shrink and swell by different amounts, so the joint between them opens. It is common in framed houses and can be filled with SBR-cement mortar and a strip of fibre mesh across the joint, as long as it is not wider than 3 mm and the column itself is not cracked.

What does a diagonal crack from a window corner mean?

A short, thin one is stress gathering at the corner of the opening and can be filled once it stops moving. A long one that steps across the brickwork, is wider at one end or runs towards a corner of the house is settlement and needs an engineer before anyone fills it.

Why is there a horizontal crack under the roof slab on the top floor?

The roof slab heats up in the sun and moves more than the brick wall under it, so a straight line opens along the joint. BIS SP 25 describes this in top storeys. Fill it with something that can move, with mesh, and keep the roof cool and dry from above.

Can wall putty fill cracks?

Only hairline ones. Birla White says putty fills minor cracks; for non-structural cracks up to 5 mm it sells a separate crack filler, Seep Guard Crack End. Joint cracks and deeper cracks need SBR-cement mortar.

The crack came back after filling. What now?

Stop filling it. Whatever opened it is still moving. Mark its ends with a pencil and the date, photograph it with a scale, and have an engineer look at it. How to watch it: is the crack dangerous?

Abhishek Ranjan
Diploma Civil Engineer, Tashya Ventures

Civil engineer at our Reva Road store, Muzaffarpur, for cement, steel and building questions. The causes on this page follow the Bureau of Indian Standards crack handbook; every width and product claim was checked against the maker's own page on 12 Nov 2026. Where the makers disagree, the page says so and uses the safer figure.

Where the facts come from

  1. Bureau of Indian Standards, SP 25 (1984), Handbook on causes and prevention of cracks in buildings: shrinkage cracks in plaster, cracks at the joint of RCC frame and brick walls, horizontal cracks under the roof slab in top storeys from the slab's heat movement, diagonal cracks from foundation movement.
  2. UltraTech, How to repair cracks in walls: hairline cracks under 1 mm usually cosmetic; settlement cracks wider at one end; over 3 mm needs a professional check; professional help above 1 cm in the repair steps; keep concrete repairs damp for 3 days.
  3. Dr. Fixit, Wall crack repair: structural vs superficial cracks: call a structural engineer for cracks wider than 3 mm; diagonal cracks from openings and recurring cracks as warning signs.
  4. Asian Paints, Movement cracks vs structural cracks: width alone is not a reliable guide; check place, direction and change over time.
  5. Birla White, Seep Guard Crack End: polymer-modified white-cement crack filler for non-structural cracks up to 5 mm.
  6. Birla White, Wall putty basics: putty fills minor cracks and holes; WallCare FAQ: not a levelling material.
  7. ISO/IEC 7810 (ID-1 card): bank and ATM cards are 0.76 mm thick.

Send us a photo of the crack

With an ATM card beside it and one photo of the whole wall. We'll tell you which card it matches and what fills it, with today's price.