Terrace and roof waterproofing for a house already built: what to do, in what order, and what makes it last

The short answer
  1. Clean
  2. Repair cracks
  3. Fix slope and outlets
  4. Round the parapet corner
  5. Hi-Flex × 2, crosswise
  6. Screed or tiles on top

The coating is a skin less than a millimetre thick. What makes it last is the roof under it (no open cracks, no water standing) and the layer over it (screed or tiles that keep the sun and feet off). Skip either, and a good coating fails in a few seasons.

~7 sq ft
Per kg, both coatsUltraTech: 1 kg Hi-Flex covers 14–15 sq ft for one coat. Two coats take double.
8 h
Between coats, at leastThe second coat runs at right angles to the first.
1 in 100
Slope to the outletAt least 1¼ inch fall over 10 ft. Usual practice.
A finished roof, parapet to outlet
Cross-section of a waterproofed terrace The roof slab with a crack cut open and filled, a low spot filled, a rounded mortar corner at the parapet, two coats of Hi-Flex carried one foot up the parapet and into the outlet, a sloping screed on top with tiles on part of it, and the parapet top sloped inwards. RCC ROOF SLAB slope ≥ 1 in 100, to the outlet 1 FT ROOM BELOW · CEILING STAYS DRY 1 2 3 4 5 6 7 Hi-Flex coat 1 Hi-Flex coat 2, crosswise Screed, sloped Terrace tiles (optional) Repair mortar with WP+200
  1. Cracks cut into a V and filled with WP+200 mortar.
  2. Low spots built up so no water stands.
  3. Outlet cleared, set low, coating carried into its mouth.
  4. Gola: a rounded mortar corner where slab meets parapet.
  5. Hi-Flex, two coats, crosswise, 1 ft up the parapet.
  6. Screed on top with the slope; tiles on it if the roof is used.
  7. Parapet top sealed and sloped towards the roof.
Not to scale: each Hi-Flex coat is only 0.6–0.7 mm. Coats, gap and screed: UltraTech Weather Pro brochure. Slope, gola and 1 ft upturn: usual practice.
Before you buy anything

Walk the roof the day after rain, with a piece of chalk

On a flat roof in Bihar, water that stands is the first cause of failure. You see it best a few hours after rain. Mark every problem with chalk, take photos, and you have the repair list.

Your roof from above: what to mark
Plan of a flat roof with problems marked A rectangular roof inside its parapet. Two outlets on the right side. Arrows show the slope running to the outlets. A pond of water left after rain, chalk circles round cracks, a hollow patch, a water tank on a stand with pipes, and the parapet corner all round marked as a joint to seal. hollow A B C D E F
  1. Outlets: at least two, clear, set lower than the roof round them.
  2. Pond: water still standing hours after rain.
  3. Cracks: ring each one with chalk.
  4. Hollow patch: sounds dull when tapped with a hammer handle.
  5. Tank legs, pipes, dish and solar bolts: every hole through the roof.
  6. Parapet corner, all round: where most roof leaks start.

BPour a bucket, wait an hour

On a dry day, pour a bucket of water near the middle and watch where it goes. Any puddle still there after an hour is a low spot. It must be built up, or the new coating will fail there first.

CHairline or wide?

Fine cracks in the top surface are normal and get filled. A crack you can push a coin into, one that runs right through to the ceiling, or one that keeps growing, needs looking at first: structural or plaster crack?

DTap for hollow patches

Old plaster, IPS or old coating that sounds dull has come loose underneath. Cut it out back to sound concrete. Don't hammer off layers that are still sound: breaking up an old roof can crack the slab.

ACount the outlets

One outlet means one blocked pipe floods the whole roof. Usual practice is at least two, with one 4-inch pipe for roughly every 400–500 sq ft of roof.

FLook at the parapet, top and bottom

Water gets in where the slab meets the wall, and through cracks on top of the parapet that let rain run down inside the wall.

EEvery hole through the roof

Pipe sleeves, tank-stand legs, cable holes, dish and solar-panel bolts. Each one gets packed and coated round, or it leaks no matter how good the coating is.

Is water dripping into a room right now? Stop it first, then come back to this page in a dry spell: chhat se pani tapak raha hai. Send the chalk-marked photos to us on WhatsApp and we'll go through them with you.

The method

Eight steps, in this order, on a dry roof

Do the whole roof, not only the spot that leaked: water moves to the next weakest point. Plan for about a week of dry weather, plus curing for the screed.

Clean down to a sound surface

Sweep, scrape off moss, loose plaster and any old coating that is lifting. Wash with water, brush out the dust and let the roof dry. Every coating maker puts poor surface preparation first among the causes of failure.

Check: the roof is dry to the touch and even in colour before any coat goes on.

Open and fill the cracks

Cut each chalk-marked crack into a small V with a chisel or grinder and brush it out. Wet it, brush in a cement and SBR slurry, then press in cement–sand mortar made with WP+200. Keep it damp for a few days.

Use: WP+200, 200 ml per 50 kg bag, added to the second half of the mixing water. Seal & Dry SBR slurry: ratio from the pack. Moving cracks: joints and cracks.

Build up the low spots

Brush SBR slurry on the old surface, then lay WP+200 mortar to fill every puddle mark so water runs on to the outlets. Keep the fill at least ¾ inch (20 mm) thick; mortar feathered to nothing cracks and lifts.

If the whole roof is flat or slopes the wrong way, the slope is made in the screed at step 8 instead.

Fix the outlets

Clear the pipe right through. Make a shallow dish (khurra) round each outlet mouth, about an inch lower than the roof, so the last water drains away. Fit a jali cap to keep out leaves and plastic. Add a second outlet if there is only one.

Usual practice: at least two outlets; one 4-inch pipe for about 400–500 sq ft.

Round the parapet corner, seal every hole

Run a gola, a rounded fillet of WP+200 mortar about 2–3 inches, along the foot of the parapet so the coating never bends round a sharp corner. Pack the gaps round pipe sleeves, tank legs and bolts with SBR mortar.

Parapet details: parapet waterproofing. Tank stand: tank platform on the roof.

Hi-Flex, coat 1

Mix the powder and liquid of Hi-Flex as the pack says and brush the first coat over the whole roof, the gola, 1 ft up the parapet, round every pipe, and 3–4 inches into each outlet mouth. Aim for 0.6–0.7 mm.

Use: UltraTech Weather Pro Hi-Flex, 12 or 24 kg. 1 kg covers 14–15 sq ft for this coat.

Hi-Flex, coat 2, at right angles

After at least 8 hours, brush the second coat across the first: if coat 1 ran north–south, coat 2 runs east–west. The crossing fills the pinholes and thin streaks a single coat always leaves.

Another 14–15 sq ft per kg. Let it set as the pack says before anyone walks on it.

Test it, then cover it

Block the outlets with a cloth bag of sand, pond about an inch of water for 24–48 hours (usual practice) and check the ceiling below. Then lay the screed with the slope to the outlets, and tiles on it if the roof is used. Cure the screed at least 10 days, 14 in hot dry weather.

Screed: UltraTech cement with WP+200, or Weather Plus on its own. One or the other, not both. Choices below.
Why the second coat runs across
Two coats laid crosswise On the left, one coat of brush strokes running one way, with pinholes and thin streaks between strokes. On the right, the second coat laid at right angles covers them. At least 8 hours between the coats, each 0.6 to 0.7 mm. ≥ 8 h Coat 1 onlyCoat 2, across it pinholes and thin streaksgaps coveredEach coat 0.6–0.7 mm (UltraTech)
The outlet, done properly
Section through a roof outlet A vertical rainwater pipe through the slab. Around its mouth the screed dips into a shallow dish about an inch lower than the roof. The coating runs down into the pipe mouth three to four inches. A domed jali cap sits on top. ~1 in lower khurra (dish) jali cap coating 3–4 ininto the pipe 4-inch pipe, at leasttwo outlets per roof
What goes on top

Screed or tiles over the coating: why and which

UltraTech's own brochure says it is "highly recommended" to lay a screed or plaster over Hi-Flex. Sun, feet, a water tank and the odd dropped brick are what wear a roof coating out. Here are the three choices, worst to best.

Short life

Bare coating

Only for a roof nobody walks on
  • Takes the full sun and every footstep. Expect to inspect it every year and recoat sooner.
  • Nothing heavy on it: no tank stand, no drying racks, no chairs.
  • Never on a roof that still holds water anywhere.
Good

Screed

Cement–sand mortar over the coating
  • Usual practice 1:4 cement–sand, about 1–1½ inch on average, thicker at the high side to make the slope.
  • Made with UltraTech PPC and WP+200 (200 ml a bag), or with Weather Plus on its own. Not both.
  • Cure at least 10 days, 14 in hot dry weather, as for any cement work.
Best for a roof you use

Screed plus tiles

Drying clothes, sitting out, children playing
  • Outdoor anti-skid tiles such as Birla Pivot 400×400 outdoor (11.8 mm, 5 tiles = 8.61 sq ft a box). More choices: terrace tiles.
  • Lay them in WP+200 mortar on the screed, or with Birla White TileStix Extero adhesive (we order it for you). TileStix Intero Grip+ is for indoors only.
  • Fill every joint, and leave a small gap at the parapet so the tiles can move in the heat.
How long it lasts

The roof decides how long it lasts, more than the brand

Contractor and brand sites quote roughly 5 to 15 years for terrace waterproofing. That is a range, not a promise for your roof. Where your job lands in that range depends on four things.

What wears a coating out
Bare coating compared with a covered coating Left: a bare coating hit by sun, feet and standing water, with cracks and a lifted blister. Right: the same coating under a screed and tiles; the sun, feet and water stop at the top layer and the coating stays whole. Bare coatingUnder screed and tiles sun cracks itfeet scuff itwater standsand lifts it screed and tiles take the wear,the coating stays whole
Not to scale. The point: a coating lasts by being kept out of the sun and from under people's feet.
What decides itLong lifeShort life
Water on the roofthe biggest one on flat Bihar roofsAll water reaches the outlets within an hourPuddles stand for days after rain
Cover on topUltraTech recommends oneScreed, or screed and tilesBare coating in the sun
PreparationCracks filled, loose layers cut out, roof clean and dryCoated over dust, moss or lifting plaster
Coats and cornersTwo crosswise coats, gola, 1 ft up the parapet, round every pipeOne coat, sharp corners, holes left
What the makers' warranties say
  • UltraTech Hi-Flex: the Weather Pro brochure gives the coverage, coats and 100% stretch, but no warranty period.
  • Birla White Seep Blocker 2K: 3 years on waterproofing, with a registration form on Birla White's site.
  • Dr. Fixit: quotes 7 to 12 years on its Roofseal range, applied by its own contractors.
A product warranty is about the product, not about a roof with puddles. Keep the GST bill and register where the maker asks.
Every year, before the monsoon (about 30 minutes) Clear the outlets and jali caps. Look at the parapet top and the gola for new cracks. Re-pack any sleeve or bolt that has opened. Never drill into the roof for a dish, solar stand or railing without sealing the hole the same day. Full list: before the monsoon.
What goes wrong

Six ways a good coating fails early

We see the same six on roofs around Muzaffarpur. Every one is cheaper to avoid than to redo.

ONE COAT

One coat instead of two

You see: damp spots that come back in patches

A single brushed coat always has pinholes and thin streaks. UltraTech asks for two, the second at right angles, at least 8 hours later.

NO COVER

Nothing laid over the coating

You see: worn, cracked coating in a few seasons

Sun and feet go straight at it. UltraTech highly recommends a screed or plaster on top. On a roof you use, tiles on that screed.

PONDING LEFT

A low spot left as it was

You see: the leak returns right under the old puddle

Water standing for days softens and lifts any coating. Fill the dip and fix the slope before coating, not after.

DUST UNDER IT

Coated over dust, moss or loose plaster

You see: the coating peels off in sheets

It sticks to the dust, not to the roof. Dr. Fixit names poor surface preparation as the most common waterproofing mistake. Scrape, wash, dry.

PARAPET JOINT MISSED

Coating stopped at the parapet corner

You see: a damp band along the top of the wall inside

The slab and wall move differently and the joint opens. Make a gola, carry both coats 1 ft up the parapet, and seal the parapet top.

RAIN TOO SOON

Coated on a damp roof, or rain came too soon

You see: streaks, soft patches, white bloom

Start only when the roof is dry and no rain is expected for the whole job: 8 hours for coat 1, then coat 2. In winter, wait until the dew has dried.

Also seen: waterproof putty or paint on the ceiling inside. Waterproof putty does not stop water that is getting in; fix the roof, let the ceiling dry, then see painting a wall that was damp.

How much to buy

Material for your roof

Put in the roof size inside the parapet. Hi-Flex uses UltraTech's figure (14–15 sq ft per kg for each coat, two coats). Screed figures are usual practice. Packs are chosen for the high number.

Area to coat: — sq ft

Your list

UltraTech Weather Pro Hi-Flex, 2 coats—1 kg covers 14–15 sq ft for one coat at 0.6–0.7 mm (UltraTech). Packs 12 and 24 kg.—

Prices are from our latest bill and change often. Please confirm today's rate on WhatsApp or call before buying.

UltraTech cement, screed
—1:4 cement–sand screed, usual practice, plus 2 bags for cracks, gola and low spots—
Sand, screed—For the same 1:4 mix. We deliver sand too.Ask today's rate
Weather Pro WP+200—200 ml per 50 kg bag of cement in the repair mortar and screed (UltraTech). Skip it if you use Weather Plus.—
Seal & Dry SBR1 kgBond slurry for cracks, sleeves and the outlet. More if large areas are being built up.Buy: 1 × 1 kg · Ask rate
Birla Pivot 400×400 outdoor tiles—8.61 sq ft per box (Birla Pivot), plus 5% for cuttingAsk today's rate per box
Material totalAsk rate
Send this list on WhatsApp

Prices are filled in from today's rate. Cutting and delivery are charged separately; ask for the amount for your site (delivery). Bathrooms and tanks: waterproofing calculator. Worked examples: how much Hi-Flex.

Questions people ask us

Short answers

How long does terrace waterproofing last?

It depends more on the roof than on the product. Contractor and brand sites quote roughly 5 to 15 years. A coating under a screed or tiles, on a roof where all water reaches the outlets, lasts at the long end. A bare coating in the sun on a roof that holds water lasts at the short end. UltraTech gives no warranty period for Hi-Flex; Birla White gives 3 years on Seep Blocker 2K.

Can I just paint a waterproof coat on a leaking terrace?

Not on its own. Each coat is only 0.6–0.7 mm. On open cracks, standing water, a sharp parapet corner or a dusty surface it fails early. Repair, slope and clean first, then two coats, then a cover. If it is dripping now, start with chhat se pani tapakna.

How many coats of Hi-Flex does a terrace need?

Two, each 0.6–0.7 mm, at least 8 hours apart, the second at right angles to the first. 1 kg covers 14–15 sq ft for one coat, so the job takes about 1 kg for every 7 sq ft.

How much Hi-Flex for a 1000 sq ft roof?

About 134–143 kg for two coats, which is six 24 kg packs, plus a little more for the parapet upturn. The calculator above works it out for your roof.

Do I need tiles or screed over the coating?

UltraTech says it is highly recommended to lay a screed or plaster over Hi-Flex. It keeps sun, feet and the water tank's weight off the coating. If the roof is used every day, put tiles on that screed.

Can it be done in the rain, or in winter?

Not in the rain or on a wet roof. Winter is fine on dry days once the morning dew has dried. The best time in Muzaffarpur is March to May, before the monsoon.

My terrace already has old tiles or china mosaic. Can I coat over them?

UltraTech's brochure doesn't cover coating over glazed tiles, so we don't advise it. Tap every tile: lift the hollow and cracked ones, fill the gaps with WP+200 mortar, and if most are loose, take them up and do the full method. If the tiles are all sound and the leak is at the parapet or an outlet, fix those details first.

Hi-Flex or Seep Blocker 2K for the roof?

Hi-Flex for the whole roof: it comes in 12 and 24 kg and stretches up to 100% by UltraTech's figures. Seep Blocker 2K (3 kg) for a small area such as a tank top, a corner or a patch. See Hi-Flex vs Seep Blocker 2K.

Who will apply the waterproofing near me?

A careful mason can do this job by following the eight steps above. Send us photos of your roof, the outlets and the parapet corners on WhatsApp and we will look at them with you and send the list of material. Before you hire anyone: questions to ask a waterproofing thekedar.

Mr Mustafaa
Paint Engineer, Tashya Ventures

Paint Engineer at our Reva Road store, Muzaffarpur, and our waterproofing advisor. Every maker's figure on this page was checked against the maker's own published sheet on 12 Nov 2026. Where a figure is usual practice rather than a maker's, the page says so.

Where the numbers come from

  1. UltraTech, Weather Pro waterproofing brochure: Hi-Flex for terraces and roofs, 0.6–0.7 mm per coat, 1 kg covers 14–15 sq ft, two coats at least 8 hours apart with the second perpendicular, screed or plaster "highly recommended" on top, elongation up to 100%, up to 7 bar, packs 12 and 24 kg. WP+200: 200 ml per 50 kg bag, added to the second half of the mixing water. No warranty period is given.
  2. Birla White, Seep Blocker 2K page: two-part coating of white cement, silica sand and acrylic polymer, up to 5 bar, elongation up to 90%, 3-year waterproofing warranty with registration.
  3. Dr. Fixit, waterproofing cost and application guide: poor surface preparation named the most common mistake; and the roof waterproofing page: Roofseal warranties of 7 to 12 years.
  4. Birla Pivot catalogue: 400×400 outdoor tile, 11.8 mm, 5 tiles = 8.61 sq ft per box. Birla White: TileStix Intero Grip+ indoors only; Extero for outdoor tiles.
  5. IS 456: curing at least 10 days for cement work, 14 in hot dry weather. Slope, outlet count, gola size, screed mix and ponding test: usual practice, labelled as such.
  6. Coverage per coat: UltraTech prints 14–15 sq ft per kg next to a 0.6–0.7 mm coat, so we count it per coat and double it for two coats. That way you do not run short halfway.

Send us photos of your roof

The whole roof, the outlets and the parapet corners, with the rough size. We'll look at them with you and send the material list with today's price on WhatsApp.

TASHYABUILDING SOLUTIONS · MUZAFFARPUR
WhatsApp 90310 74624tashyaventures.com