हिंदी Call90310 74624
Home›Bihar›Waterproofing
Bihar homes · before the monsoon

Roof leaking? What to check before the monsoon, and how to stop it

The short answer
  1. Check in the dry months
  2. Chalk every fault
  3. Fix each one its own way
  4. Coat the whole roof only if it has failed

A flat roof in Bihar leaks at the same eight places, and most of them are not cracks. Find them on a dry roof, any time from October to May, and repair each one. A coating over an unrepaired roof, or a coat put on in the rain, does not last. Finish everything by the end of May.

8
Places to checkKhurra, parapet joint, cracks, low spots, pipes, tank base, sariya, mumty door.
10–15 Jun
Normal monsoon onsetFor Bihar, as the Met office gives it. Plan to finish two weeks before.
2 coats
Of Hi-Flex, if the roof needs itAt least 8 hours apart, crosswise, then a screed over it (UltraTech).

Water dripping today? This page is for planning the repair. For what to do while it rains, read chhat se pani tapak raha hai: the emergency steps.

Where a Bihar roof lets water in
Eight places a Bihar roof lets water in Side view of a flat-roofed house with a stair cabin (mumty) and a water tank on top. Numbered: 1 khurra outlet blocked with leaves, 2 joint where the parapet meets the slab, 3 hairline crack in the slab, 4 low spot where rain water stands, 5 pipe through the slab, 6 base of the tank platform with the overflow pipe dropping water on it, 7 sariya left sticking up for the next floor, 8 low door step of the mumty. Damp patches show on the ceiling of the room below. Check on a dry, sunny day,October to May ROOM BELOW damp patches show on the ceiling 1 2 3 4 5 6 7 8 1 2 3 4 5 6 7 8 Khurra (outlet) blocked Parapet–slab joint Crack in the lenter Low spot, water stands Pipe through the slab Tank platform base Sariya for next floor Mumty door step
The far parapet is drawn behind the roof so the khurra shows. The patch on the ceiling is often a little away from the point where water gets in.
When to do it

A roof is mended in the dry months, not in the rain

Most people climb up only when the ceiling drips. By then nothing can be done properly. Three reasons to go up now.

1Coatings need a dry roof

Hi-Flex, repair mortar and screed all have to grip clean, dry concrete. On a wet roof the coat does not bond, and the money is gone with the next rain.

2The faults show best now

In October and November the stains from the rains are still on the ceiling, so you know where to look. By April the long heat has opened the hairline cracks wide enough to see.

3The full job takes two weeks

Repairs have to cure, the two Hi-Flex coats need at least 8 hours between them, and a screed is kept damp for about a week. That needs a run of dry days, which June cannot promise.

The Met office gives 10 to 15 June as the normal date the monsoon reaches Bihar. Count back two weeks of work and a little spare: the last safe start is mid-May. What else to do that month is on the April page.

The roof year in north Bihar

Two good windows, one last call

When to check and mend a roof in Bihar, month by month October and November: read the fresh stains and repair. December and January: cold, foggy mornings, work later in the day on a dry surface. February and March: good working weather for the full job. April and May: last call, finish the coating and screed by 31 May. Early June is risky; the monsoon normally reaches Bihar on 10 to 15 June. June to September: rains, no coating; keep the khurras clear and chalk new stains. OctNovDecJanFebMarAprMayJunJulAugSep Read this year's stains Cold, foggy mornings Good working weather Last call Rains: no coating, no screed Ceiling marks are still fresh.Repair cracks and joints now. Work late morning to afternoon,only on a surface dry to touch. The full job: repairs, 2 coats,screed. Needs two dry weeks. Heat opens hairline cracks.Finish coat and screed by 31 May. Keep khurras clear. Chalk-marknew stains on the ceiling forthe October check. Monsoon reaches Bihar ~10–15 June goodwith carelast callrain

October and November are the best time to find leaks. The rains have just ended, the roof dries fast, and every stain on the ceiling is a map of where water got in this year. Walk the roof now, chalk the faults, and do the repairs while you remember them.

December and January are workable, with care. North Bihar mornings are foggy and the roof is wet with dew until late morning. Start after the surface feels dry and stop before evening, so nothing is laid on a damp slab.

February to May is the main season. Most people get the whole job done in March or April. In May the roof is very hot in the afternoon; work in the morning and keep the fresh mortar damp.

June to September, leave the coating alone. If it leaks, patch it for now (emergency steps), keep the khurras clear, and mark every new stain with a pencil date. Those marks are your October list.

The roof check · one morning

Walk the roof in this order and chalk what you find

Take a broom, a bucket or hose, white chalk, a screwdriver and your phone. Sweep first: you cannot see a crack under dust and leaves. Then wet the roof lightly and wait half an hour. Cracks stay dark longest, and the low spots keep their water.

BroomBucket or hoseWhite chalkScrewdriverPhone camera
Your roof after the check
Top view of a roof marked with chalk after the check Top view of a flat roof inside its parapet. The khurra is in the bottom-left corner and grey arrows show the slope towards it. Chalk lines mark the parapet edge, two cracks, the outline of a pond in the middle, a ring around a pipe, the tank platform on the mumty, a group of four sariya ends, and the mumty door. Each mark carries the number of the check. MUMTY 1 2 3 4 5 6 7 8 3 grey arrows: the way water should run, to the khurra
1

Khurra (outlet)

Look: leaves, mud, a plastic bag, a mouth that sits higher than the roof. Test: pour a bucket near it. It should run away in a clear stream.

Fix 1 · clear and reset

2

Parapet joint

Look: along the foot of every parapet and the mumty wall: a hairline gap, white powder, black lines. Test: scratch with a screwdriver; loose mortar means open joint.

Fix 2 · gola and coat up the wall

3

Cracks in the slab

Look: after wetting, thin lines that stay dark when the rest has dried. Mark: chalk the whole length, and note any you can put a coin edge into.

Fix 3 · open, fill, strip-coat

4

Low spots

Look: half an hour after wetting, patches where water still stands, or old rings of dirt and green moss. Mark: chalk the outline.

Fix 4 · slope it to the khurra

5

Pipes through the slab

Look: a gap or crumbling ring where a pipe, a cable or a dish stand passes through. Test: press around it with the screwdriver.

Fix 5 · collar and coat

6

Tank platform

Look: cracks where the brick platform meets the roof, and where the overflow pipe empties. A wet patch at the base all year is the sign.

Fix 6 · fillet, coat, move the overflow

7

Sariya for the next floor

Look: bars left sticking up for a future storey. Rust running down them, and cracks in the concrete around their base.

Fix 7 · seal and cap the bars

8

Mumty door step

Look: a step that is level with the roof, or water marks on the stairs inside. Roof water runs straight in under the door.

Fix 8 · raise the step

Also rub the old coating, if there is one, with your palm. Powder on the hand, flakes, or bare patches mean it has worn out: see whole roof or not. Then go downstairs and photograph every ceiling stain. Send the photos with your chalk marks to us on WhatsApp if you want a second look.

The fix, fault by fault

Each fault has its own repair

These are spot repairs. Do every one you chalked, on a dry roof, before any coating goes on the whole roof. In the drawings the layers are drawn much thicker than they are.

SBR slurry (bond coat) Mortar with WP+200 Hi-Flex coat Water
1 Clear leaves and mud2 Set the mouth a little belowthe roof, in WP+200 mortar3 Coat into the mouth, add a grating slope runs to the khurra →

1 · Khurra blocked or set high

You see: water standing in the corner
  1. Clear it and pour a bucket. If it drains, you are done.
  2. If water stands at the mouth, chip around it and reset the mouth a little lower than the roof, in mortar with WP+200 (200 ml per 50 kg bag of cement).
  3. Take the Hi-Flex coat into the mouth and fit a grating.

One khurra for a big roof is a common cause of standing water. How many a roof needs: roof drainage.

at least 1 ft up the wallgola: rounded cornerand about 1 ft out on the roofsloped cap on top

2 · Parapet joint open

You see: stains along the wall edge of the ceiling
  1. Rake out loose mortar along the joint and brush it clean.
  2. Brush on SBR slurry, then build a rounded gola (fillet) of mortar with WP+200 in the corner, about a palm wide (usual practice).
  3. When it has cured, coat Hi-Flex from about a foot out on the roof to at least a foot up the wall.

Do the mumty walls the same way. Parapet top and cracks in its plaster: parapet waterproofing.

1 Open into a V, dust off2 SBR slurry, 3 WP+200 mortar4 Hi-Flex strip,2 coats over it keep the filling damp for a few days before coating

3 · Hairline cracks

You see: a straight-line stain on the ceiling
  1. Open each crack into a small V with a chisel and blow the dust out.
  2. Brush SBR slurry into the groove and fill it with mortar made with WP+200, while the slurry is still tacky.
  3. Keep it damp for a few days, then coat a strip of Hi-Flex over it, two coats.

A crack you can put a coin edge into, or one that has grown since last year, needs a look first: structural or minor?

Fill the dip with sloping mortar(SBR slurry under, WP+200 in it)khurra water used to stand here fall of about 1 inch every 8 ft (usual practice)

4 · Low spots and standing water

You see: a round patch that grows after rain
  1. Clean the area, brush on SBR slurry so the new layer sticks to the old slab.
  2. Lay cement mortar with WP+200, sloped so water runs to the khurra. A fall of about 1 inch in every 8 feet is usual practice.
  3. Keep it damp, then test with a bucket: nothing should stand after an hour.

No coating survives water that stands on it for days. This is the step people skip most.

1 Rake out the gap2 SBR slurry3 Cone of WP+200 mortar4 Hi-Flex over thecollar and up the pipe

5 · Pipes through the slab

You see: a patch around a pipe on the ceiling
  1. Rake out the loose ring around the pipe.
  2. Brush SBR slurry on the pipe and the concrete, then pack a sloping cone collar of mortar with WP+200, so water runs away from the pipe.
  3. Coat Hi-Flex over the collar and a little way up the pipe.

Same for dish antenna stands, solar frames and old tent-peg holes from a wedding shamiana.

overflow pipeto the khurrafillet and Hi-Flex all round the platform base

6 · Tank platform

You see: a patch under the tank, wet all year
  1. Fix any leaking tank fitting first, or the patch never dries.
  2. Make a small gola of mortar with WP+200 all round the platform base, then coat Hi-Flex up its sides and onto the roof.
  3. Run the overflow pipe to the khurra, not onto the roof.

Tank itself seeping: water tank waterproofing.

1 Wire-brush the rust2 SBR slurry on the bars3 Mortar cone, WP+2004 Cap each bar5 Hi-Flex overthe cone

7 · Sariya left for the next floor

You see: rust stains, cracks round the column top
  1. Wire-brush the loose rust off the bars and the concrete at their base.
  2. Brush SBR slurry on, then build a sloping cone of mortar with WP+200 round the base of the bars.
  3. Coat Hi-Flex over the cone and cap each bar end so rain does not run down it.

Do not cut the bars if you plan to build up. Rust on bars: sariya par jang.

Step built up above the roof,roof sloped away from the doorwater now runs awaystairs inside

8 · Mumty door step

You see: water on the stairs after rain
  1. Build the step up in mortar with WP+200 so it stands clearly above the finished roof (2 to 3 inches is usual practice).
  2. Make sure the roof near the door slopes away from it.
  3. Seal the gap under the door frame with SBR mortar.

If you will lay a screed on the whole roof, plan the step height after the screed, not before.

Whole roof or not

Decide how much your roof needs

Spot repairs are cheap; a full coat is not. Your chalk marks and the palm test on the old surface decide which one is right.

Spot repairs only

Old surface sound, a few marks, leaks in one or two places
Repairs 1–8Hi-Flex strips on repairs
  • Do only the fixes you chalked.
  • Coat a strip of Hi-Flex over each repair, two coats.
  • Check again next October.

Repairs plus an edge band

Stains only along the walls; the middle of the roof is fine
RepairsGola all roundHi-Flex band, 1 ft + 1 ft
  • Gola at every parapet and mumty wall.
  • Hi-Flex band: about 1 ft on the roof and at least 1 ft up the wall, all round.
  • Parapet tops capped: parapet page.

The whole roof

Old coat powdery or peeling, many cracks, standing water, or leaks in several rooms
All repairsHi-Flex × 2Screed
  • All repairs and slope first.
  • Two coats of Hi-Flex over the whole roof and up the walls.
  • A screed over it, as UltraTech recommends. The order and waits are below.
A coat is a skin. On a roof that still holds water or has open cracks, it fails in a season or two.
The whole roof, layer by layer
Layers of a fully waterproofed roof at the parapet Cut-away at the parapet: the roof slab with cracks repaired and an SBR slurry bond coat, a rounded mortar gola at the corner, Hi-Flex coat 1, Hi-Flex coat 2 laid across the first, both carried at least a foot up the parapet, and a screed of mortar with WP+200 on top. An inset shows coat 2 running across coat 1. ≥ 1 ft coat 2 runs across coat 1 1 2 3 4 5 numbers match the table · not to scale
Coat thickness, gap and the screed come from UltraTech's Weather Pro brochure. Gola size, the height up the wall and screed mix are usual practice.
StepWait
1 · All spot repairsSBR slurry, then mortar with WP+200 at 200 ml per 50 kg bag of cement (UltraTech). Slope fixed.few days damp
2 · Gola at every wallParapets and mumty, same mortar, rounded.cured
3 · Hi-Flex coat 1Mix the powder and liquid together. 0.6–0.7 mm thick, up the walls at least 1 ft.≥ 8 h
4 · Hi-Flex coat 2At right angles to coat 1 (UltraTech).dry, per pack
5 · Screed on topUltraTech "highly recommends" a screed or plaster over the coat. Usual practice: 1:4 cement-sand, about 20 mm, WP+200 in the water, sloped to the khurras.7 days damp
Count about two weeks of dry days. Never coat a damp roof or just before rain. In May, coat in the early morning, not on a slab too hot to touch. If the roof will be used for drying grain or for functions, the screed matters even more: feet and sun wear a bare coat away. Step-by-step method for a new or existing roof: terrace waterproofing and roof waterproofing in the house-building guide.
How much to buy

Hi-Flex, cement and WP+200 for your roof

Put in the roof size inside the parapet. Hi-Flex uses the safe reading of UltraTech's figure (see the note under the list), so you will not run short halfway.

Area to coat: — sq ft (roof plus wall strip, two coats)

Your list

Weather Pro Hi-Flex, 2 coats—1 kg covers 14–15 sq ft per coat (UltraTech), so two coats take double—
Cement for the screed—1:4 mortar, about 20 mm thick (usual practice), plus sand—
Weather Pro WP+200—200 ml per 50 kg bag of cement (UltraTech)—
Seal & Dry SBR, for repairsby repairsDepends on how many cracks and joints you chalked. Mix it with cement as printed on the pack.Start with 1 kg · Ask rate
Material totalAsk rate
Send this list on WhatsApp

Why double: UltraTech's brochure gives 14–15 sq ft per kg and 0.6–0.7 mm a coat, without saying whether the area is for one coat or both. One coat is the only reading that fits that thickness, so we count two coats as double. Prices fill in from today's rate. Tank, bathroom or wall: waterproofing calculator.

Questions people ask us

Short answers

How do I stop water dripping from the roof for good? (chhat se pani tapakna kaise roke)

Find every place the water gets in, using the eight checks above, and fix each one on a dry roof. If the old surface has failed, then give the whole roof two coats of Hi-Flex and a screed over it. A coat over unrepaired faults does not last.

What should I check on the roof before the rains?

Sweep, pour water at each khurra, walk the parapet joint, wet the roof and chalk the cracks and the spots where water stays, then check the pipes, the tank platform, any sariya sticking up and the mumty door step. Downstairs, photograph every ceiling stain.

When should roof waterproofing be done in Bihar?

Any time from October to May, on a dry roof. October and November are best for finding leaks; April and May are the last call. The monsoon normally reaches Bihar around 10 to 15 June, and the full job needs about two weeks of dry days, so finish by the end of May.

Can it be done now, in winter?

Yes, on dry days. Wait until the dew and fog have gone and the surface is dry to the touch, usually by late morning, and stop before the evening damp. Do not coat a slab that feels cold and wet.

What is the treatment for leakage in an old roof? (purani chhat ki leakage)

Repair first: cracks, parapet joint, slope, pipes, khurra. If the old coating is powdery or peeling, or water comes in at many places, coat the whole roof with two coats of Hi-Flex laid crosswise and put a screed over it, as UltraTech's brochure recommends.

Does filling the cracks alone stop the leak?

Only if the cracks were the only fault. On most Bihar roofs we also find an open parapet joint, a blocked khurra or a low spot where water stands. Check all eight.

Which waterproofing chemical is best for a roof?

Each one does a different job. A flexible coating like Weather Pro Hi-Flex goes on top. WP+200 is not a coating: it goes in the water of the repair mortar and screed, 200 ml per 50 kg bag. Seal & Dry SBR makes the bond coat so new mortar sticks to the old slab. People who ask for "Dr. Fixit Roofseal" are asking for a flexible roof coating; the one we sell is Hi-Flex.

How much Hi-Flex for a 1000 sq ft roof?

UltraTech says 1 kg covers 14–15 sq ft at 0.6–0.7 mm a coat. We read that as one coat, so two coats on 1000 sq ft take about 134 to 143 kg, plus the strip up the parapet. Buy for the higher figure. The calculator above does it for your size.

How long will it last?

Contractors commonly quote 5 to 15 years for roof waterproofing; that is an industry estimate, not a promise. A coat under a screed, on a roof that drains, lasts at the long end. A bare coat in sun on a roof that holds water lasts at the short end. Check it every October either way.

Mr Mustafaa
Paint Engineer, Tashya Ventures

Paint Engineer at our Reva Road store, Muzaffarpur, and the person to ask about waterproofing. The product figures on this page were checked against UltraTech's own Weather Pro brochure on 12 Nov 2026. Where the brochure is unclear, the page says so and gives the safer figure. Figures marked "usual practice" are common site practice, not a maker's figure.

Where the numbers come from

  1. UltraTech, Weather Pro waterproofing brochure: WP+200 at 200 ml per 50 kg bag, mixed into half the water; packs 200 ml to 100 L. Hi-Flex: powder and liquid mixed, 0.6–0.7 mm a coat, two coats at least 8 hours apart, the second at right angles, 1 kg covers 14–15 sq ft, screed or plaster over it "highly recommended", up to 100% elongation (ASTM D 412), packs 12 and 24 kg.
  2. India Met Department, as reported by PTI (India TV News): normal date of monsoon arrival in Bihar, 10–15 June.
  3. Usual practice, labelled where used: gola about a palm wide, coating at least 1 ft up the wall, fall of about 1 inch per 8 ft, screed 1:4 about 20 mm, 7 days damp curing. Screed cement worked out at 1.33 dry volume, 1,440 kg per m³ of cement.
  4. Service life 5–15 years: commonly quoted by contractors, not a maker's warranty.

Send us a photo of your roof

With the roof size and your chalk marks. We'll tell you which fixes it needs and send the list with today's price on WhatsApp.

TASHYABUILDING SOLUTIONS · MUZAFFARPUR
WhatsApp 90310 74624tashyaventures.com